Specifications


Typical Tensile Properties

Condition Elongation Tensile Strength Testing Temperature Testing Time Yield Strength
Stress Relieved 29 % 95 ksi 1150 °F 1 hr 81 ksi
Stress Relieved 24 % 95 ksi 1350 °F 1 hr 82 ksi
Stress Relieved 26 % 93 ksi 1375 °F 1 hr 80 ksi

Typical Weld Metal Analysis %

wire composition
PMnCuMoX-barSCVSiNiCr
max 0.012 %0.40-0.70 %max 0.20 %0.40-0.65 %max 12 ppmmax 0.025 %0.07-0.012 %max 0.03 %0.40-0.70 %max 0.20 %1.20-1.50 %

Classifications: AWS A5.28; ER80S-B2

x

Typical Tensile Properties

Condition Elongation Tensile Strength Testing Temperature Testing Time Yield Strength
Stress Relieved 29 % 95 ksi 1150 °F 1 hr 81 ksi
Stress Relieved 24 % 95 ksi 1350 °F 1 hr 82 ksi
Stress Relieved 26 % 93 ksi 1375 °F 1 hr 80 ksi

Typical Weld Metal Analysis %

wire composition
PMnCuMoX-barSCVSiNiCr
max 0.012 %0.40-0.70 %max 0.20 %0.40-0.65 %max 12 ppmmax 0.025 %0.07-0.012 %max 0.03 %0.40-0.70 %max 0.20 %1.20-1.50 %

Classifications: AWS A5.28; ER80S-B2

x

Part Numbers and Accessories

Select All | Select None

Check box to add

Part Numbers : TIGROD ER80S-B2
NCU80SB2 5/32X36X10#T/30#CT 150JF54 FIND A DISTRIBUTOR
NCU80SB2 3/32X36X10#T/30#CT 150JF50 FIND A DISTRIBUTOR
NCU80SB2 1/8X36X10#T/30#CT 150JF52 FIND A DISTRIBUTOR
NCU80SB2 1/16X36X10#T/30#CT 150JF48 FIND A DISTRIBUTOR
x
×

Find the Closest Distributor

x

x

Loading..