Stoody NiCrMo3-T1

Stoody

Stoody NiCrMo3-T1

The following items have been added to your list


x

Stoody NiCrMo3-T1 is a gas shielded flux cored wire that can be used for welding in all positions using argon/CO2 mixtures. The wire possesses excellent weldability and can be used in a wide variety of similar and dissimilar welding and cladding applications. The iron content of the all-weld deposit is kept below 1% for applications requiring enhanced corrosion resistance.

BUY NOW


Features

  • Joining nickel-chromium-molybdenum alloys to UNS N06625. Clad side of joints in steel clad with nickel-chromium-molybdenum weld metal Surfacing steel with nickel-chromium-molybdenum weld metal Joining steels to nickel based alloys Joining 9% nickel steel for cryogenic applications

Industries

  • Petrochemical

Typical Weld Metal Analysis %

Typical Weld Metal Analysis %
Element Si C Fe Mn Cr P S Ti Co Nb+Ta Mo Ni
Nominal Percentage 0.35 % 0.02 % 0.3 % 0.2 % 21.0 % 0.005 % 0.003 % 0.1 % 0.02 % 3.3 % 8.5 % Balance %

Typical Charpy V-Notch Properties

Condition 1
Impact Value (imp) 44 ft-lb
Impact Value (met) 60 J
Testing Temperature -196 degC (-320 degF)
Condition 1
Conditional Statement ASME Testing Using 1 in. Thick 9% Ni, 3G
Impact Value (imp) 57 ft-lb
Impact Value (met) 77 J
Testing Temperature -196 degC (-320 degF)

Classifications

Grade TNi 6625-14
Name ISO
Name ENiCrMo3T1-4
Grade 2018
Name AWS A5.34/A5.34M

Typical Tensile Properties

Condition As Welded As Welded
ASME Testing Using 1 in. Thick 9% Ni, 3G, Cross-Joint
Tensile Strength (imp) 105 ksi 104 ksi
Tensile Strength (met) 725 MPa 714 MPa
Yield Strength (imp) 68 ksi
Yield Strength (met) 470 MPa
Elongation 38 %

Welding Parameters

Wire Feed Speed 735-1000
Wire Feed Speed 290-400
Wire Diameter 1.2
Wire Diameter .045
Voltage 25-27
Shielding Gas 75% - Ar/25% - CO2
Current 150-200