Purus 46
A copper coated G4Si1/ER70S-6 solid wire for GMAW of carbon-manganese steels. Purus 46 is particularly suited to be used in general construction, automotive components and mobile machinery industries. It has a slightly higher manganese and silicon content than Purus 42 to increase the weld metal strength.The wire may be welded with either a gas mixture or with pure CO2 as shielding gas. Purus 46 is designed to give a clean weld bead with a minimum of silica islands and spatter. The wire is suitable for robotic applications at high deposition rates.
Typical Charpy V-Notch Properties
Impact Value | Testing Temperature | |||
as welded aws co2 (c1) | ||||
70 J (52 ft-lb) | -30 degC (-22 degF) | |||
as welded en 80ar/20co2 (m21) | ||||
130 J (96 ft-lb) | 20 degC (68 degF) | |||
70 J (52 ft-lb) | -30 degC (-22 degF) | |||
60 J (44 ft-lb) | -40 degC (-40 degF) | |||
as welded en 92ar/8co2 (m20) | ||||
90 J (66 ft-lb) | -30 degC (-22 degF) | |||
80 J (59 ft-lb) | -40 degC (-40 degF) | |||
as welded en co2 (c1) | ||||
120 J (88.5 ft-lb) | 20 degC (68 degF) | |||
70 J (52 ft-lb) | -30 degC (-22 degF) |
Typical Tensile Properties
Condition | As Welded | As Welded | As Welded | As Welded |
Shielding Gas | EN 80Ar/20CO2 (M21) | EN CO2 (C1) | AWS CO2 (C1) | EN 92Ar/8CO2 (M20) |
Tensile Strength | 585 MPa (85 ksi) | 560 MPa (81 ksi) | 560 MPa (81 ksi) | 600 MPa (87 ksi) |
Yield Strength | 475 MPa (69 ksi) | 450 MPa (65 ksi) | 450 MPa (65 ksi) | 500 MPa (73 ksi) |
Elongation | 26 % | 26 % | 29 % | 25 % |
Deposition Data
Current | Deposition Rate | Diameter | Voltage | Wire Feed Speed |
60-200 A | 0.8-2.3 kg/h (1.8-5.1 lb/h) | 0.8 mm (0.030 in.) | 18-24 V | 3.2-10.0 m/min (126-394 in./min) |
70-250 A | 0.9-3.5 kg/h (2.0-7.7 lb/h) | 0.9 mm (0.035 in.) | 18-26 V | 3.0-12.0 m/min (118-472 in./min) |
80-300 A | 1.0-5.5 kg/h (2.2-12. lb/h) | 1.0 mm (0.040 in.) | 18-32 V | 2.7-15.0 m/min (106-591 in./min) |
100-350 A | 1.2-7.0 kg/h (2.6-15. lb/h) | 1.14 mm (0.045 in.) | 18-34 V | 2.6-15.0 m/min (102-591 in./min) |
120-380 A | 1.3-8.0 kg/h (2.9-17. lb/h) | 1.2 mm (0.047 in.) | 18-35 V | 2.5-15.0 m/min (98-591 in./min) |
130-400 A | 1.5-8.5 kg/h (3.3-18. lb/h) | 1.32 mm (0.052 in.) | 19-35 V | 2.4-15.0 m/min (94-591 in./min) |
150-420 A | 1.6-8.7 kg/h (3.5-19. lb/h) | 1.4 mm (0.055 in.) | 22-36 V | 2.3-12.0 m/min (91-472 in./min) |
225-550 A | 2.1-9.4 kg/h (4.6-20. lb/h) | 1.6 mm (1/16 in.) | 28-38 V | 2.3-10.0 m/min (91-394 in./min) |
Classifications
Wire Electrode |
SFA/AWS A5.18 : ER70S-6 EN ISO 14341-A : G 4Si1 |
Weld Metal |
EN ISO 14341-A : G 42 3 C1 4Si1 EN ISO 14341-A : G 46 4 M21 4Si1 EN ISO 14341-A : G 46 4 M20 4Si1 |
Approvals
Approvals |
CE EN 13479 DB 42.039.40 VdTÜV 19261 |
Approvals are based on factory location. Please contact ESAB for more information. |
Consumable Characteristics
Alloy Type | Carbon-manganese steel (Mn/Si-alloyed) |
Typical Weld Metal Analysis %
Wire Composition | ||||||||||||||
C | Mn | Si | ||||||||||||
0.08 % | 1.65 % | 0.90 % |
Extra Info