Coreweld 110

ESAB

Coreweld 110

The following items have been added to your list


x

Coreweld 110 is a metal cored electrode designed for single and multipass welding of high strength low alloy steels, such as T-1, HY-80, and HY-100. The arc is smooth with virtually no spatter. Coreweld 110 is recommended for welding quenched and tempered high strength steels. Because of the metallic core, the wire offers both the high deposition rates of a flux cored electrode and the high efficiencies of a solid wire.

BUY NOW


Industries

  • Bridge Construction
  • Ship/Barge Building

Welding Process

  • MCAW - Metal Core Arc Welding

Typical Charpy V-Notch Properties

Impact Value Testing Temperature
as welded 75% ar - 25% co2
47 J (35 ft-lb) -18 degC (0 degF)
41 J (30 ft-lb) -51 degC (-60 degF)

Typical Tensile Properties

ConditionElongationShielding GasTensile Strength Yield Strength
As Welded18 %75% Ar - 25% CO2773 MPa (112 ksi)662 MPa (96 ksi)

Recommended Welding Parameters

Current TTW Dist. Voltage Wire Diameter Wire Feed Speed
75% Ar - 25% CO2
150-350 A 9.5-19 mm (3/8-3/4 in.) 24-32 V 1.2 mm (.045 in.) 838-1453 cm/min (330-572 in./min)
200-400 A 9.5-19 mm (3/8-3/4 in.) 26-32 V 1.4 mm (.052 in.) 665.5-833 cm/min (262-328 in./min)
300-500 A 9.5-19 mm (3/8-3/4 in.) 26-34 V 1.6 mm (1/16 in.) 460-846 cm/min (181-333 in./min)

Deposition Data

Current Deposition Rate Diameter Deposition Efficiency (%) TTW Dist. Voltage Wire Feed Speed
75% Ar - 25% CO2
170 A 2.4 kg/h (5.2 lb/h) 1.2 mm (.045 in.) 94 % 16 mm (5/8 in.) 24 V 510 cm/min (200 in./min)
230 A 3.5 kg/h (7.7 lb/h) 1.2 mm (.045 in.) 96 % 16 mm (5/8 in.) 25 V 760 cm/min (300 in./min)
290 A 4.6 kg/h (10.2 lb/h) 1.2 mm (.045 in.) 98 % 16 mm (5/8 in.) 27 V 1020 cm/min (400 in./min)
330 A 5.8 kg/h (12.7 lb/h) 1.2 mm (.045 in.) 99 % 16 mm (5/8 in.) 29 V 1270 cm/min (500 in./min)
390 A 7.5 kg/h (16.5 lb/h) 1.2 mm (.045 in.) 99 % 16 mm (5/8 in.) 32 V 1650 cm/min (650 in./min)
190 A 2.5 kg/h (5.5 lb/h) 1.4 mm (.052 in.) 94 % 16 mm (5/8 in.) 24 V 440 cm/min (180 in./min)
240 A 3.5 kg/h (7.7 lb/h) 1.4 mm (.052 in.) 95 % 16 mm (5/8 in.) 25 V 640 cm/min (250 in./min)
310 A 4.9 kg/h (10.7 lb/h) 1.4 mm (.052 in.) 98 % 16 mm (5/8 in.) 27 V 890 cm/min (350 in./min)
370 A 6.2 kg/h (13.6 lb/h) 1.4 mm (.052 in.) 99 % 16 mm (5/8 in.) 30 V 1140 cm/min (450 in./min)
420 A 7.5 kg/h (16.6 lb/h) 1.4 mm (.052 in.) 99 % 16 mm (5/8 in.) 32 V 1400 cm/min (550 in./min)
230 A 2.81 kg/h (6.2 lb/h) 1.6 mm (1/16 in.) 91 % 19 mm (3/4 in.) 24 V 380 cm/min (150 in./min)
290 A 4.0 kg/h (8.8 lb/h) 1.6 mm (1/16 in.) 95 % 19 mm (3/4 in.) 26 V 510 cm/min (200 in./min)
370 A 5.7 kg/h (12.5 lb/h) 1.6 mm (1/16 in.) 96 % 19 mm (3/4 in.) 28 V 700 cm/min (280 in./min)
430 A 7.2 kg/h (15.9 lb/h) 1.6 mm (1/16 in.) 99 % 19 mm (3/4 in.) 29 V 890 cm/min (350 in./min)
90% Ar - 10% CO2
200 A 3.0 kg/h (6.5 lb/h) 1.2 mm (.045 in.) 95 % 16 mm (5/8 in.) 27 V 640 cm/min (250 in./min)
260 A 4.1 kg/h (9.1 lb/h) 1.2 mm (.045 in.) 97 % 16 mm (5/8 in.) 28 V 890 cm/min (350 in./min)
290 A 4.6 kg/h (10.2 lb/h) 1.2 mm (.045 in.) 98 % 16 mm (5/8 in.) 29 V 1020 cm/min (400 in./min)
330 A 5.8 kg/h (12.7 lb/h) 1.2 mm (.045 in.) 99 % 16 mm (5/8 in.) 32 V 1270 cm/min (500 in./min)
190 A 2.5 kg/h (5.5 lb/h) 1.4 mm (.052 in.) 94 % 16 mm (5/8 in.) 26 V 440 cm/min (180 in./min)
240 A 3.5 kg/h (7.7 lb/h) 1.4 mm (.052 in.) 95 % 16 mm (5/8 in.) 27 V 640 cm/min (250 in./min)
280 A 4.2 kg/h (9.2 lb/h) 1.4 mm (.052 in.) 97 % 16 mm (5/8 in.) 28 V 760 cm/min (300 in./min)
340 A 5.1 kg/h (11.2 lb/h) 1.4 mm (.052 in.) 99 % 16 mm (5/8 in.) 31 V 1020 cm/min (400 in./min)
410 A 7.1 kg/h (15.7 lb/h) 1.4 mm (.052 in.) 99 % 16 mm (5/8 in.) 36 V 1330 cm/min (530 in./min)
230 A 2.81 kg/h (6.2 lb/h) 1.6 mm (1/16 in.) 91 % 19 mm (3/4 in.) 26 V 380 cm/min (150 in./min)
290 A 4.0 kg/h (8.8 lb/h) 1.6 mm (1/16 in.) 95 % 19 mm (3/4 in.) 27 V 510 cm/min (200 in./min)
340 A 5.6 kg/h (12.3 lb/h) 1.6 mm (1/16 in.) 98 % 19 mm (3/4 in.) 29 V 640 cm/min (250 in./min)
510 A 9.4 kg/h (20.7 lb/h) 1.6 mm (1/16 in.) 99 % 19 mm (3/4 in.) 36 V 1210 cm/min (480 in./min)
360 A 6.3 kg/h (13.9 lb/h) 1.2 mm (.045 in.) 99 % 16 mm (5/8 in.) 33 V 1400 cm/min (550 in./min)
430 A 7.2 kg/h (15.9 lb/h) 1.6 mm (1/16 in.) 99 % 19 mm (3/4 in.) 32 V 890 cm/min (350 in./min)

Classifications

Classifications ASME SFA 5.36 :
ASME SFA 5.28 :
AWS A5.36 : E110T15-M21A6-K3-H4
AWS A5.28 : E110C-K3

Typical Weld Metal Analysis %

Typical Weld Metal Analysis %
C Mn Mo Ni P S Si
75% Ar - 25% CO2
0.07 % 1.6 % 0.5 % 2.3 % 0.01 % 0.02 % 0.35 %
x

Part Numbers and Accessories

Select All | Select None

Check box to add

Part Numbers : Coreweld 110
243415882 FIND A DISTRIBUTOR
243416187 FIND A DISTRIBUTOR
243416138 FIND A DISTRIBUTOR
243416120 FIND A DISTRIBUTOR
243416179 FIND A DISTRIBUTOR

ESAB EQUIPMENT WARRANTIES ARE VALID ONLY WHEN PURCHASED THROUGH AN ESAB AUTHORIZED DEALERSHIP.

x
x

x

Loading..