Dual Shield II 81-K2
The wire produces a smooth stable arc and low spatter levels using a 100% CO2 shielding gas. Dual Shield II 81-K2 was developed for higher tensile steels such as ASTM A302, A533 Class I and A537. Applications include ship fabrication, offshore oil rigs, and heavy equipment construction. This wire is an excellent choice for welding ASTM steels A302, A533 Class I and A537. Dual Shield II 81-K2 produces a smooth stable arc and low spatter levels using 100% CO2 shielding gas. Applications include ship building, offshore oilrigs, and heavy equipment construction.
Industries
- Civil Construction
- Industrial and General Fabrication
- Mobile Equipment
- Railcars
- Ship/Barge Building
Welding Process
- FCAW (Flux Core)
Typical Weld Metal Analysis %
Typical Weld Metal Analysis % | ||||||||||||||
C | Mn | Ni | P | S | Si | |||||||||
100% CO2 | ||||||||||||||
.025 % | 1.18 % | 1.44 % | 0.013 % | 0.009 % | 0.49 % |
Approvals
Approvals |
ABS 5Y400SA H5 BV SA5Y50/SA5Y40 H5 CCS 5Y42SH5 CE EN 13479 ClassNK KSWL3G(C)H5, KSW54Y40G(C)H5 (C1) DNV V Y40MS H5 (C1) GL 6Y40H5S (C1) KR L3SG(C) H5 & 5Y40SG(C) H5 LR 5Y40S H5 (C1) RINA 5YS H10 (C1) RS 5Y40S H5, 5Y50S H5 (C1) |
Approvals are based on factory location. Please contact ESAB for more information. |
Typical Charpy V-Notch Properties
Impact Value | Testing Temperature |
136 J(100 ft-lb) | -18 degC(0 degF) |
121 J(89 ft-lb) | -29 degC(-20 degF) |
81 J(60 ft-lb) | -51 degC(-60 degF) |
Classifications
ASME SFA 5.29 : ASME SFA 5.36 : AWS A5.36 : E81T1-C1A6-K2-H8 AWS A5.29 : E81T1-K2C-H8 |
Consumable Characteristics
Welding Current | DC+ |
Diffusible Hydrogen | < 4 ml/100g |
Alloy Type | C Mn Ni |
Typical Tensile Properties
Condition | Elongation | Reduction in Area | Shielding Gas | Tensile Strength | Yield Strength |
As Welded | 27 % | 73 % | 100% CO2 | 570 MPa (82 ksi) | 515 MPa (74 ksi) |
Recommended Welding Parameters
Current | TTW Dist. | Voltage | Wire Diameter | Wire Feed Speed |
100% CO2 | ||||
135-205 A | 9.5-12.7 mm(3/8-1/2 in.) | 23-26 V | 1.2 mm(.045 in.) | 381-660 cm/min(150-260 in./min) |
205-230 A | 12.7-19 mm(1/2-3/4 in.) | 25-27 V | 1.2 mm(.045 in.) | 660-965 cm/min(260-380 in./min) |
230-265 A | 19-25.4 mm(3/4-1 in.) | 26-30 V | 1.2 mm(.045 in.) | 965-1321 cm/min(380-520 in./min) |
125-235 A | 12.7-16 mm(1/2-5/8 in.) | 23-26 V | 1.4 mm(.052 in.) | 279-584 cm/min(110-230 in./min) |
235-290 A | 16-19 mm(5/8-3/4 in.) | 25-29 V | 1.4 mm(.052 in.) | 584-864 cm/min(230-340 in./min) |
290-350 A | 19-25.4 mm(3/4-1 in.) | 29-31 V | 1.4 mm(.052 in.) | 864-1194 cm/min(340-470 in./min) |
165-270 A | 16-19 mm(5/8-3/4 in.) | 25-28 V | 1.6 mm(1/16 in.) | 279-508 cm/min(110-200 in./min) |
270-345 A | 19-25.4 mm(3/4-1 in.) | 27-30 V | 1.6 mm(1/16 in.) | 508-762 cm/min(200-300 in./min) |
345-415 A | 25.4-31.75 mm(1-1.25 in.) | 28-32 V | 1.6 mm(1/16 in.) | 762-1067 cm/min(300-420 in./min) |
Deposition Data
Current | Deposition Rate | Diameter | Efficiency (%) | Voltage | Wire Feed Speed |
100% CO2 | |||||
150 A | 1.91 kg/h(4.2 lb/h) | 1.2 mm(.045 in.) | 86 % | 28 V | 508 cm/min(200 in./min) |
210 A | 2.86 kg/h(6.3 lb/h) | 1.2 mm(.045 in.) | 86 % | 29 V | 762 cm/min(300 in./min) |
250 A | 3.86 kg/h(8.5 lb/h) | 1.2 mm(.045 in.) | 87 % | 30 V | 1016 cm/min(400 in./min) |
245 A | 3.31 kg/h(7.3 lb/h) | 1.4 mm(.052 in.) | 86 % | 28 V | 635 cm/min(250 in./min) |
310 A | 4.63 kg/h(10.2 lb/h) | 1.4 mm(.052 in.) | 85 % | 33 V | 889 cm/min(350 in./min) |
360 A | 6.03 kg/h(13.3 lb/h) | 1.4 mm(.052 in.) | 85 % | 36 V | 1143 cm/min(450 in./min) |
300 A | 4.63 kg/h(10.2 lb/h) | 1.6 mm(1/16 in.) | 87 % | 30 V | 635 cm/min(250 in./min) |
365 A | 5.58 kg/h(12.3 lb/h) | 1.6 mm(1/16 in.) | 86 % | 33 V | 762 cm/min(300 in./min) |
410 A | 6.35 kg/h(14 lb/h) | 1.6 mm(1/16 in.) | 88 % | 33 V | 889 cm/min(350 in./min) |
155 A | 2.00 kg/h(4.4 lb/h) | 1.4 mm(.052 in.) | 87 % | 25 V | 381 cm/min(150 in./min) |
190 A | 2.77 kg/h(6.1 lb/h) | 1.6 mm(1/16 in.) | 87 % | 27 V | 38 cm/min(150 in./min) |