Arcaloy 308L-17 Plus electrodes have a heavy coating, produce a concave bead with minimum ripple and the slag is virtually self-cleaning. These electrodes are designed to weld Types 304, 304L, 321 and 347 for corrosion service at temperature up to about 315°C (600°F). The excellent wetting action and very fine ripple minimize crevice corrosion and grinding time. This is particularly useful in the food and drink industry where a smooth polished surface is required.

BUY NOW


Industries

  • Food and Beverage
  • Railcars
  • Industrial and General Fabrication
  • Ship/Barge Building

Specifications


Typical Tensile Properties

Elongation Tensile Strength Yield Strength
(in 2") 47 % 86 ksi 58 ksi

Welding Parameters

Flat Amps Overhead Amps Vertical Amps Wire Diameter
20-35 A 20-30 A 15-25 A 1.6 mm
30-50 A 30-40 A 25-35 A 2.0 mm
60-85 A 40-60 A 40-60 A 2.4 mm
90-120 A 60-85 A 70-80 A 1/8 in.
140-165 A 95-120 A 80-90 A 4.0 mm
180-210 A 125-150 A 100-115 A 3/16 in.
205-290 A - - 1/4 in.

Typical Weld Metal Analysis %

weld metal analysis
MnMoCuCSiFerriteNiCr
0.6 %0.1 %0.1 %0.02 %0.8 %6 FN %10 %19 %

Approvals: AWS A5.4; E308-17/E308L-17; ASME IX F No. 5; E308-17/E308L-17; ASME II SFA A5.4; CWB; CSA W48 E308L-17

Approvals are based on factory location. Please contact ESAB for more information.


x

Typical Tensile Properties

Elongation Tensile Strength Yield Strength
(in 2") 47 % 86 ksi 58 ksi

Welding Parameters

Flat Amps Overhead Amps Vertical Amps Wire Diameter
20-35 A 20-30 A 15-25 A 1.6 mm
30-50 A 30-40 A 25-35 A 2.0 mm
60-85 A 40-60 A 40-60 A 2.4 mm
90-120 A 60-85 A 70-80 A 1/8 in.
140-165 A 95-120 A 80-90 A 4.0 mm
180-210 A 125-150 A 100-115 A 3/16 in.
205-290 A - - 1/4 in.

Typical Weld Metal Analysis %

weld metal analysis
MnMoCuCSiFerriteNiCr
0.6 %0.1 %0.1 %0.02 %0.8 %6 FN %10 %19 %

Approvals: AWS A5.4; E308-17/E308L-17; ASME IX F No. 5; E308-17/E308L-17; ASME II SFA A5.4; CWB; CSA W48 E308L-17

Approvals are based on factory location. Please contact ESAB for more information.


x

Part Numbers and Accessories

Select All | Select None

Check box to add

Part Numbers : ARCALOY 308L-17 PLUS
AC 308L-17 1/8X14X10# 251035366 FIND A DISTRIBUTOR
AC 308L-17 3/16X14X10#HS 251035382 FIND A DISTRIBUTOR
AC 308L-17 3/32X12X8#HS 251035358 FIND A DISTRIBUTOR
AC 308L-17 5/32X14X10#HS 251035374 FIND A DISTRIBUTOR
x
×

Find the Closest Distributor

x

x

Loading..