Typical Tensile Properties

90% Ar - 10% CO2
Condition Elongation Tensile Strength Yield Strength
As Welded 22 % 85 ksi 72 ksi
75% Ar - 25% CO2
Condition Elongation Tensile Strength Yield Strength
As Welded 21 % 85 ksi 71 ksi

Typical Charpy V-Notch Properties

90% Ar - 10% CO2
Condition Impact Value Testing Temperature
As Welded 65 ft-lb -50 °F
As Welded 84 ft-lb -40 °F
As Welded 96 ft-lb -20 °F
75% Ar - 25% CO2
Condition Impact Value Testing Temperature
As Welded 58 ft-lb -50 °F
As Welded 60 ft-lb -40 °F
As Welded 73 ft-lb -20 °F

Typical Weld Metal Analysis %

ELEMENTVALUES
PMnMoCuSCVSiNiCr
0.011 %1.18 %0.01 %0.16 %0.007 %0.09 %0.004 %0.58 %0.02 %0.03 %

Deposition Data

Spray Transfer
Diameter Current Deposition Rate Voltage Wire Feed Speed
.030 in.
0.8 mm
160 A 5.8 lb/h
2.6 kg/h
24 V 500 in./min
1270 cm/min
.035 in.
0.9 mm
180 A 6.3 lb/h
2.9 kg/h
25 V 400 in./min
1016 cm/min
.030 in.
0.8 mm
173 A 6.4 lb/h
2.9 kg/h
25 V 550 in./min
1397 cm/min
.035 in.
0.9 mm
197 A 7.1 lb/h
3.2 kg/h
26 V 450 in./min
1143 cm/min
.030 in.
0.8 mm
187 A 7 lb/h
3.2 kg/h
25 V 600 in./min
1524 cm/min
.035 in.
0.9 mm
213 A 7.9 lb/h
3.6 kg/h
26 V 500 in./min
1270 cm/min
.030 in.
0.8 mm
200 A 7.6 lb/h
3.4 kg/h
26 V 650 in./min
1651 cm/min
.035 in.
0.9 mm
230 A 8.7 lb/h
4 kg/h
27 V 550 in./min
1397 cm/min
.045 in.
1.2 mm
260 A 7.9 lb/h
3.6 kg/h
25 V 300 in./min
762 cm/min
.045 in.
1.2 mm
280 A 9.2 lb/h
4.2 kg/h
26 V 350 in./min
889 cm/min
.045 in.
1.2 mm
300 A 10.5 lb/h
4.8 kg/h
28 V 400 in./min
1016 cm/min
.045 in.
1.2 mm
320 A 11.8 lb/h
5.4 kg/h
29 V 450 in./min
1143 cm/min
.045 in.
1.2 mm
340 A 13.1 lb/h
6 kg/h
30 V 500 in./min
1270 cm/min

Deposition Data

Short Arc Transfer
Diameter Current Deposition Rate Voltage Wire Feed Speed
.035 in.
0.9 mm
160 A 4.6 lb/h
2.1 kg/h
19 V 300 in./min
762 cm/min
.030 in.
0.8 mm
80 A 2.2 lb/h
1 kg/h
15 V 200 in./min
508 cm/min
.035 in.
0.9 mm
90 A 2.7 lb/h
1.2 kg/h
15 V 180 in./min
457 cm/min
.030 in.
0.8 mm
100 A 2.8 lb/h
1.3 kg/h
15 V 250 in./min
635 cm/min
.030 in.
0.8 mm
120 A 3.3 lb/h
1.5 kg/h
16 V 300 in./min
762 cm/min
.030 in.
0.8 mm
140 A 3.9 lb/h
1.8 kg/h
16 V 350 in./min
889 cm/min
.045 in.
1.2 mm
130 A 3.1 lb/h
1.4 kg/h
17 V 125 in./min
318 cm/min
.045 in.
1.2 mm
163 A 4 lb/h
1.8 kg/h
18 V 160 in./min
406 cm/min
.045 in.
1.2 mm
200 A 5 lb/h
2.3 kg/h
19 V 200 in./min
508 cm/min
.035 in.
0.9 mm
113 A 3.3 lb/h
1.5 kg/h
16 V 220 in./min
559 cm/min
.030 in.
0.8 mm
144 A 4 lb/h
1.8 kg/h
16 V 350 in./min
914 cm/min
.035 in.
0.9 mm
137 A 4 lb/h
1.8 kg/h
18 V 260 in./min
660 cm/min
.030 in.
0.8 mm
60 A 1.7 lb/h
0.8 kg/h
14 V 150 in./min
381 cm/min

Approvals: ABS; AWS A5.18: ER70S-3 H4; CWB CSA W48; CAN/CSA-ISO14341,B-G 49A 2C G3 (ER49S-3); MIL-E-23765/1 MIL-70S-3
Classifications: AWS A5.18; ER70S-3 H4

Approvals are based on factory location. Please contact ESAB for more information.


x
×

Find the Closest Distributor

x

Find the Closest Distributor

x

x

Loading..