This site uses cookies and other tracking technologies to provide you with our services, enhance the performance and functionality of our services, analyze the use of our products and services, and assist with our advertising and marketing efforts.

Cookie Policy   Privacy Notice

Previous Next

ESAB

CORESHIELD 40

Typical Tensile Properties

Condition Elongation Tensile Strength Yield Strength
As Welded 29 % 86 ksi 62 ksi

Typical Weld Metal Analysis %

ELEMENTVALUES
PMnSCSiAl
0.012 %0.30 %0.007 %0.20 %0.30 %1.30 %

Deposition Data

Diameter Current Deposition Rate Efficiency (%) Electrical Stickout Voltage Wire Feed Speed
5/64 in.
2.0 mm
220 A 6 lb/h
2.7 kg/h
77 % 1.75 in.
44.5 mm
27 V 120 in./min
305 cm/min
5/64 in.
2.0 mm
300 A 9.4 lb/h
4.26 kg/h
85 % 1.75 in.
44.5 mm
28 V 178 in./min
452 cm/min
5/64 in.
2.0 mm
400 A 11.6 lb/h
5.26 kg/h
84 % 1.75 in.
44.5 mm
29 V 230 in./min
584 cm/min
3/32 in.
2.4 mm
350 A 13.8 lb/h
6.26 kg/h
82 % 2.5 in.
63.5 mm
28 V 196 in./min
498 cm/min
3/32 in.
2.4 mm
375 A 15.1 lb/h
6.85 kg/h
84 % 2.5 in.
63.5 mm
29 V 212 in./min
539 cm/min
3/32 in.
2.4 mm
400 A 116.1 lb/h
7.3 kg/h
84 % 2.5 in.
63.5 mm
30 V 229 in./min
582 cm/min

Classifications: ASME SFA 5.36; AWS A5.36; E70T4-Z-CS3; ASME SFA 5.20; AWS A5.20; E70T-4