ESAB

DUAL SHIELD T-115

DUAL SHIELD T-115

Dual Shield T-115 is a basic slag flux cored electrode designed for applications requiring a high strength weld deposit. Dual Shield T-115 produces weld deposits which are resistant to cracking in heavy sections or under high restraint. It has good usability with a minimum amount of spatter and easy slag removal. It can be used for welding steels such as: T-1, HY-80, HY-90, N-A-XTRA 90, 100 and 110, and the SSS 100 series. The weld metal analysis is similar to an E11018-M low hydrogen electrode. A 100% CO2 shielding gas is recommended for the 3/32" (2.4 mm) size and a 75% Ar / 25% CO2 gas for the .045 " (1.2 mm) and 1/16" (1.6 mm) sizes.

Where To Buy


Industries

  • Industrial and General Fabrication
  • Mobile Equipment

Welding Process

  • Welding-FCAW - Flux Core Arc Welding

Specifications


Typical Tensile Properties

75% Ar - 25% CO2
Condition Elongation Reduction in Area Stress Relieved Temperature Stress Relieved Testing Time Tensile Strength Yield Strength
Stress Relieved 23 % 65 % 1050 °F 1 hr 109 ksi 96 ksi
100% CO2
Condition Elongation Reduction in Area Stress Relieved Temperature Stress Relieved Testing Time Tensile Strength Yield Strength
As Welded 22 % 57 % - - 96 ksi 117 ksi
75% Ar - 25% CO2
Condition Elongation Reduction in Area Stress Relieved Temperature Stress Relieved Testing Time Tensile Strength Yield Strength
As Welded 20 % 43 % - - 118 ksi 110 ksi

Typical Charpy V-Notch Properties

75% Ar - 25% CO2
Condition Impact Value Stress Relieved Testing Temp Stress Relieved Testing Time Testing Temperature
Stress Relieved 48 ft-lb 1050 °F 1 hr -20 °F
Stress Relieved 32 ft-lb 1050 °F 1 hr -60 °F
As Welded 50 ft-lb - - -20 °F
As Welded 36 ft-lb - - -60 °F

Typical Weld Metal Analysis %

75% Ar - 25% CO2
PMnMoSCSiNiCr
0.010 %1.86 %0.47 %0.012 %0.05 %0.52 %2.04 %0.25 %
100% CO2
PMnMoSCSiNiCr
0.011 %1.86 %0.44 %0.012 %0.06 %0.56 %2.11 %0.44 %

Approvals: CWB; CSA W48 E111T5-K4M-H4 (.045”,.052”,1/16”), E110T5-K4C-H4 (3/32”)
Classifications: ASME SFA 5.36; ASME SFA 5.29; AWS A5.36; E111T5-M21A6-K4-H4 (.045”, .052”, 1/16”); AWS A5.36; E110T5-C1A6-K4-H4 (3/32"); AWS A5.29; E110T5-K4C (3/32"); AWS A5.29; E111T5-K4M-H4 (.045", .052", 1/16")