Purus 42

Typical Tensile Properties

100% CO2
Condition Elongation Tensile Strength Yield Strength
As Welded 24 % 77 ksi 62 ksi
80% Ar - 20% CO2
Condition Elongation Tensile Strength Yield Strength
As Welded 25 % 81 ksi 68 ksi

Typical Charpy V-Notch Properties

100% CO2
Condition Impact Value Testing Temperature
As Welded 48 ft-lb -40 °F
As Welded 55 ft-lb -22 °F
As Welded 81 ft-lb 68 °F
80% Ar - 20% CO2
Condition Impact Value Testing Temperature
As Welded 59 ft-lb -40 °F
As Welded 66 ft-lb -22 °F
As Welded 96 ft-lb 68 °F

Typical Weld Metal Analysis %

PMnSCSi
0.020 %1.45 %0.020 %0.085 %0.85 %

Deposition Data

Diameter Current Deposition Rate Voltage Wire Feed Speed
1/16 in.
1.6 mm
225-550 A 4.6-20.7 lb/h
2.1-9.4 kg/h
28-38 V 90-395 in./min
2.3-10 m/min
0.052 in.
1.4 mm
150-420 A 3.5-19.2 lb/h
1.6-8.7 kg/h
22-36 V 90-470 in./min
2.3-12 m/min
0.035 in.
0.9 mm
70-250 A 2.0-7.7 lb/h
0.9-3.5 kg/h
18-26 V 120-475 in./min
3.0-12 m/min
0.040 in.
1.0 mm
80-300 A 2.2-12.1 lb/h
1.0-5.5 kg/h
18-32 V 105-590 in./min
2.7-15 m/min
0.045 in.
1.2 mm
120-380 A 2.9-17.6 lb/h
1.3-8.0 kg/h
18-35 V 100-590 in./min
2.5-15 m/min
0.030 in.
0.8 mm
60-200 A 1.8-5.1 lb/h
0.8-2.3 kg/h
18-24 V 125-395 in./min
3.2-10 m/min

Approvals: CWB, CSA W48-14, VdTÜV, 19190, CE EN, 13479
Classifications: EN ISO 14341-A:, G 3Si1, SFA/AWS A5:18:, ER70S-6

Approvals are based on factory location. Please contact ESAB for more information.


Alloy Type: Carbon-manganese steel (Mn/Si-alloyed)