2 Table 5-1 – Mild Steel and Low Alloy Steel Wires Chemical Composition Requirements* (Percent – Balance Iron) SPOOLARC AWS DESIG- CLASS NATION CARBON MANG. SILICON SULFUR PHOS. MOLYB. OTHER ER70S-2 65 0.07 0.90-1.40 0.40-0.70 0.035 0.025 -- 0.05-0.15 Ti 0.02-0.12 Zr 0.05-0.15 AI ER70S-3 29S or 82 0.06-0.15 0.90-1.40 0.45-0.75 0.035 0.025 -- ER70S-4 85 0.07-0.15 1.00-1.50 0.65-0.85 0.035 0.025 -- ER70S-5 -- 0.07-0.19 0.90-1.40 0.30-0.60 0.035 0.025 -- 0.50-0.90 AI ER70S-6 86 0.07-0.15 1.40-1.8 0.80-1. I 5 0.035 0.025 -- ER70S-7 87HP 0.07-0.15 1.50-2.00 0.50-0.80 0.035 0.025 -- ERSOS-D2 83 or Hi84 0.07-0.12 1.60-2.10 0.50-0.80 0.035 0.025 0.40-0.60 ER70S-G -- NOT SPECIFIED * *Requirements are those agreed to by the purchaser and supplier.