46 Stainless
Steel Cored Wires* Typical Mechanical
Typical Undiluted Type
Properties Weld
Metal Analysis Specifications
As Welded % wt
Core-Bright 307
AWS A5.22 Tensile
Strength Carbon 0.1
ASME SFA 5.22 95,000
psi (655 MPa) Manganese 3.8
Class E307T0-3 Yield
Strength Silicon 0.6
64,000 psi (441 MPa)) Chromium
19.5 % Elongation
in 2" (51 mm) Nickel 9.8
37 Molybdenum
1.0 For welding
armor plate or carbon to stainless. Core-Bright
308Mo AWS A5.22 Tensile
Strength Carbon 0.025
ASME SFA 5.22 98,000
psi (676 MPa) Manganese 1.6
Class E308MoT0-3 Yield
Strength Silicon 0.8
67,000 psi (462 MPa)) Chromium
21.0 % Elongation
in 2" (51 mm) Nickel 10.1
37 For welding
armor plate or carbon to stainless. Continued
on next page... Recommended Welding
Parameters page 50 Additional Stainless
Cored Wires listed on page 49