3 Typical
Mechanical Typical Undiluted
Type Properties
Weld Metal Analysis Specifications
As Welded % wt
Arcaloy 308L Plus
AWS A5.4 Tensile
Strength Carbon 0.02
ASME SFA 5.4 83,700
psi Manganese 0.7
Class E308/308L-17 (577
MPa) Silicon 0.8
% Elongation in 2" (51 mm) Chromium
19.5 52
Nickel 10.0
FN 8
Arcaloy 308L Plus electrodes have a heavy coating, produce
a concave bead with minimum ripple and the slag is virtually self-
cleaning. For welding types 304, 304L, 308 and 308L when
bead appearance is important. The excellent wetting action and very
fine ripple minimize crevice corrosion and grinding time.
The low carbon content helps to prevent carbide precipitation. Arcaloy
308/308H AWS A5.4
Tensile Strength Carbon
0.04-0.08 ASME
SFA 5.4 80,000 to 90,000 psi
Manganese 1.7
Class (552 to
621 MPa) Silicon 0.5
E308/308H-15 & -16 %
Elongation in 2" (51 mm) Chromium
19.8 MIL Class
for 308-15 40 to 50 Nickel
9.6 & -16
(not L grades) ABS-E308/308H-16
FN 6
Arcaloy 308/308H can be used in all the applications
specified for 308. In addition, it can be used to weld type 304H and similar
applications where improved creep strength is required.
Carbon content 0.04% minimum. Recommended
Welding Parameters page 14 Additional Stainless
Cored Wires listed on page 13