®COPYRIGHT
2000 THE ESAB GROUP, INC. LESSON
VI 6.6.4
Spoolarc
86 (AWS
Class ER70S-6)
- Spoolarc 86 is a copper plated gas-metal
arc welding wire. Containing
a high level of deoxidizers, it produces sound welds in all carbon
steels using CO2
shielding gas, argon/CO2 and argon/O2
mixtures. The arc is quiet and very stable.
High speed, high deposition welds can be made with argon-oxygen gas mixtures.
Ideal for welding sheet metal where
smooth weld beads with good wetting action are desir- able.
It may be used to weld carbon steels that have a moderate amount of rust
or mill scale. Spoolarc
86 can also be used for out-of-position welding with the short-circuit transfer
method, making
it ideal for pipe welding. Other applications are for bridges, building
construction, boiler
and pressure vessels, storage tanks, auto parts, and construction equipment.
A. Typical
Chemical Analysis
of the
Wire Carbon
0.09% Phosphorus
0.012% Manganese
1.18% Sulfur
0.011% Silicon
0.57% B.
Typical
Mechanical Properties
of the
Weld Metal
Using CO2
Shielding Gas
Yield Point, psi
68,000 Tensile
Strength, psi 81,600
% Elongation (2")
30 Charpy
V-Notch Impacts 31
ft.-lbs. @-20°F 6.6.5
Spoolarc
87HP (AWS
Class ER70S-7)
- Spoolarc 87HP is a high manganese
carbon steel wire. It features
an optimized manganese to silicon ratio to produce excellent
appearing welds over a wide range of
welding parameters. It also produces excellent weld
metal mechanical properties and welds
over moderate amounts of rust and scale. A.
Typical
Chemical Analysis
of the
Wire Carbon
0.11% Phosphorus
0.015% Manganese
1.75% Sulfur
0.014% Silicon
0.65% B.
Typical
Mechanical Properties
of the
Weld Metal
Using 75%
Ar/25% CO2
Yield Point,
psi
66,800 Tensile
Strength, psi 79,100
% Elongation (2")
29 Charpy
V-Notch Impacts 62
ft.-lbs. @-20°F